410 is a hardenable, martensitic stainless steel containing ~12% chromium. It offers high strength and wear resistance with moderate corrosion resistance, and remains magnetic in both annealed and heat‑treated conditions. Typical uses include cutlery, fasteners, pump/valve components, and turbine parts.

Standards & Designations

  • UNS: S41000
  • EN / W. Nr.: 1.4006
  • AMS: 5504 (sheet/plate)
  • ASTM/ASME: A240/SA240 (plate, sheet, strip); A276/A479 (bars)

Corrosion resistance

Performs well in atmospheric, fresh water, and weakly acidic environments (e.g., diluted acetic, nitric, sulfuric); also resistant to food acids. Susceptible to chloride attack in oxidizing conditions; not a substitute for 304/316 in aggressive chloride service. Maximum corrosion resistance is achieved in hardened and polished conditions.

Heat treatment

  • Full anneal: 815–900 °C (1500–1650 °F); slow cool to ~600 °C (1100 °F) then air cool.
  • Process anneal: 650–760 °C (1350–1450 °F); air cool.
  • Hardening: 925–1010 °C (1700–1850 °F); air or oil quench (oil for heavy sections). Temper typically 200–400 °C to target hardness; avoid 400–580 °C to reduce embrittlement.
  • Welding

  • Machining: Readily machined in annealed or highly tempered states; machining difficulty increases above ~30 HRC (consider 416 for improved machinability if properties permit).
  • Forming: Ductile and formable in annealed condition; avoid hot working below ~899 °C (1650 °F).
  • Welding: Preheat ~150–260 °C (302–500 °F) recommended; post‑weld anneal reduces cracking. Use E/ER410 fillers for matched properties, or 309/nickel‑base fillers for ductility in as‑welded joints.
  • JCQ_slide_closeup

    Typical applications

    The list of applications for this general purpose grade is very extensive and includes:

    Chemical Composition (%)

    GradeCMnPSSiCrNiFe
    4100.08–0.151.0 max.04 max.030 max1.0 max11.5–13.5.075 maxBalance

    Mechanical properties (annealed)

    Yield Strength .2% Offset
    (psi)
    Ultimate Strength
    (psi)
    Elongation in 2”
    (%)
    Hardness
    (Rb)
    Elastic modulus
    (psi)
    30,00065,000209628.5–29 × 10⁶ psi

    Other properties

    Specific Heat
    (BTU/lb-°F)
    Electrical
    Resistivity at 68⁰F
    (μΩ-cm)
    Poisson’s RatioSpecific Gravity
    0.1155–600.27–0.307.7–7.8