347
347, also known as Type 347, is a niobium-stabilized austenitic stainless steel designed to provide excellent intergranular corrosion resistance after exposure to elevated temperatures. By stabilizing the alloy with niobium (columbium), 347 prevents chromium carbide precipitation, making it especially suitable for welded structures that operate in the 800–1500°F (427–816°C) range.
Standards & Designations
- UNS: S34700
- EN / W. Nr.: 1.4550
- ASTM/ASME: A240 (plate); A276 (bars)
Corrosion resistance
347 provides corrosion resistance comparable to Type 304, with the added benefit of resistance to sensitization and intergranular attack after welding or exposure to high temperatures. It performs well in oxidizing environments, though it is less resistant than molybdenum-bearing grades in chloride environments.
Heat treatment
347 is not hardenable by heat treatment. It is typically supplied in the annealed condition, heated to about 1900–2050°F, followed by rapid cooling. Stabilization with niobium eliminates the need for post-weld annealing in most applications.
Welding
- Machining: Similar to Type 304 but slightly more difficult due to stabilization elements.
- Forming: Good ductility allows standard forming methods.
- Welding: Excellent weldability without risk of carbide precipitation; post-weld heat treatment is generally unnecessary.
Typical applications
The list of applications for this general purpose grade is very extensive and includes:
- aerospace exhaust systems
- heat exchangers
- refinery piping
- chemical processing equipment
- boiler components
- high-temperature welded assemblies
Chemical Composition (%)
| Grade | C | Mn | Si | P | S | Cr | Ni | Nb + Ta |
|---|---|---|---|---|---|---|---|---|
| 347 | .08 max | 2.0 max | .75 max | .045 max | .030 max | 17.0–19.0 | 9.0–13.0 | 0.30-1.00 |
Mechanical properties (annealed)
| Yield Strength .2% Offset (psi) | Ultimate Strength (psi) | Elongation in 2” (%) | Elastic modulus (psi) |
|---|---|---|---|
| 30,000 | 75,000 | 40 | 28×10⁶ |
Other properties
| Density (lb/in³) | Melting Range | Electrical Resistivity at 68⁰F (μΩ-cm) | Thermal Expansion 70⁰ – 800⁰F (In/In/⁰F×10‾⁶) | Thermal Conductivity (BTU./ft.₂/hr./⁰F/ft) |
|---|---|---|---|---|
| 0.290 | 2550–2650°F | 72 | 9.2 | 9.6 |