17-4 PH
17‑4 PH, also known as Type 630, is a precipitation‑hardening martensitic stainless steel offering an exceptional combination of high strength, hardness, and moderate to good corrosion resistance. The alloy is supplied in the solution‑annealed condition (Condition A) and achieves its properties through low‑temperature aging, forming copper‑rich precipitates that dramatically increase strength.
17‑4 PH maintains high mechanical performance up to 600°F (316°C) and is widely used where high strength and corrosion resistance must coexist with reliable fabrication characteristics.
Standards & Designations
- UNS: S17400
- EN / W. Nr.: 1.4542
- AMS: 5604 (plate), 5643 (bars)
- ASTM/ASME: A564/A564M (bars), A693 (plate)
Corrosion resistance
17‑4 PH provides corrosion resistance comparable to Type 304 stainless steel in many environments and significantly superior to the hardenable 400‑series grades. Its resistance is excellent in atmospheric and mild chemical service, though susceptibility to chloride stress‑corrosion cracking increases at peak strength conditions. For chloride‑bearing environments, the alloy should be aged to the highest temperature compatible with the required strength to reduce hardness and improve SCC resistance.
Material should not be used in the annealed (Condition A) state due to lower corrosion performance.
Heat treatment
17‑4 PH uses a simple precipitation‑hardening heat‑treatment sequence, beginning with solution annealing at about 1900°F (Condition A) followed by aging between 900°F and 1150°F to achieve the desired strength and toughness. Lower aging temperatures like 900°F, produce the highest strength, while higher temperatures such as 1100–1150°F improve toughness and stress‑corrosion‑cracking resistance. The alloy should not be used long‑term above about 572°F, as elevated exposure reduces mechanical performance.
Welding
- Machining: Machinability is excellent in the solution‑annealed condition, permitting complex cutting operations.
- Forming: Being a martensitic precipitation‑hardening stainless steel, 17‑4 PH has lower ductility than austenitic grades, making forming operations more limited.
- Welding: Can be welded using standard stainless‑steel processes, typically in the solution‑annealed Condition A, and requires re‑solution annealing followed by aging to fully restore strength and corrosion resistance.
Typical applications
The list of applications for this general purpose grade is very extensive and includes:
- aerospace components
- oil & gas processing equipment
- chemical processing vessels
- food & beverage process equipment
- pulp & paper mill equipment
- mechanical components
- nuclear waste
- power generation components
Chemical Composition (%)
| Grade | C | Mn | Si | P | S | Cr | Ni | Cu | Nb + Ta |
|---|---|---|---|---|---|---|---|---|---|
| 17-4 PH | .04 max | .40 max | .50 max | .020 max | .005 max | 15.5 | 4.5 | 3.50 | 0.30 |
Mechanical properties (annealed)
| Yield Strength .2% Offset (psi) | Ultimate Strength (psi) | Elongation in 2” (%) | Impact Charpy (ft. – lbs) | Elastic modulus (psi) |
|---|---|---|---|---|
| 175,000 | 190,000 | 14 | 15 | 28.5×10⁶ |
Other properties
| Density (lb/in³) | Melting Range | Electrical Resistivity at 68⁰F (μΩ-cm) | Thermal Expansion 70⁰ – 800⁰F (In/In/⁰F×10‾⁶) | Thermal Conductivity (BTU./ft.₂/hr./⁰F/ft) |
|---|---|---|---|---|
| 0.280 | 2560–2625°F | 0.75 | 6.3 | 10.6 (at 212⁰F) |