316 / 316L
Grade 316 is a molybdenum-bearing austenitic stainless steel, offering superior corrosion resistance compared to 304, especially in chloride-rich environments. 316L is the low-carbon variant, designed to minimize carbide precipitation during welding and is often dual-certified with 316.
- 316: Offers excellent corrosion resistance and slightly higher strength, suitable for general and high-strength applications.
- 316L: Low carbon content improves weldability and prevents carbide precipitation, ideal for welded structures.
Corrosion resistance
316 resists general corrosion in marine, acidic, and polluted industrial environments.
The inclusion of ~2–3 % molybdenum significantly enhances resistance to pitting and crevice corrosion in chloride-containing media (e.g., seawater, chemical process equipment).
Heat resistance
- Continuous use: up to ~925 °C (850 °C intermittent).
- For service above ~425 °C, variants like 316H or 316Ti are preferred due to better resistance to carbide precipitation.
Heat treatment
- Annealing: 1900–2050 °F (approx. 1040–1120 °C), followed by rapid cooling to restore corrosion resistance.
- Cannot be hardened through heat treatment; instead, any strengthening is achieved via cold working.
Welding
316L, with its reduced carbon content (< 0.03 %), is ideal for welded components over ~6 mm thick, as it shows minimal sensitization and typically doesn't need post-weld annealing. Standard fillers (e.g., 316L) produce excellent weld quality.
Typical applications
The list of applications for this general purpose grade is very extensive and includes:
- chemical and petrochemical vessels
- piping
- heat exchangers
- marine equipment
- food and beverage
- medical components
- power generation
- water treatment systems
- acid processing
AISI analysis (%)
| Grade | C | Mn | P | S | Si | Cr | Ni |
|---|---|---|---|---|---|---|---|
| 316 | .08 max | 2.0 max | .045 max | .030 max | .75 max | 16.0 to 18.0 | 10.0 to 14.0 |
| 316L | .03 max | 2.0 max | .045 max | .030 max | .75 max | 16.0 to 18.0 | 10.0 to 14.0 |
Mechanical properties (annealed)
| Yield Strength .2% Offset (psi) | Ultimate Strength (psi) | Elongation in 2” (%) | Hardness (Rb) | Impact Charpy (ft. – lbs) | Elastic modulus (psi) |
|---|---|---|---|---|---|
| 28,000 – 30,000 | 75,000 – 77,000 | 40 – 42 | 80–95 | 25 | 29 × 10⁶ |
Other properties
| Creep Strength 1% Flow in 10,000 h at 1,000⁰F psi | Magnetic Permeability | Electrical Resistivity at 68⁰F (μΩ-cm) | Thermal Expansion 32⁰ – 212⁰F (In/In/⁰F×10‾⁶) | Thermal Conductivity (BTU./ft.₂/hr./⁰F/ft) |
|---|---|---|---|---|
| 17,300 | 1.01 (non‑magnetic in annealed state) | 29 | 16 × 10⁻⁶ /K | 8.1 – 9.4 (at 68⁰F) |